Analysis and Countermeasures of Cold Material Defects in Aluminum Alloy Die-Casting Specimens

Time:2026-11-16 09:31:16 / Popularity: / Source:

Die casting, as an efficient and economical metal forming technology, is widely used in automotive, aerospace, and electronic communications industries. Performance of aluminum alloy materials is a crucial foundation and guarantee in die-casting process. To verify performance of aluminum alloy materials, special molds for specimens or bars are usually developed for prototyping and tensile tests. Casting defects can affect test results, among which cold material is one of the most common defects in specimen mold, seriously interfering with accuracy of test. This study aims to systematically analyze causes of cold material defects inside specimens and explore effective prevention and improvement measures to improve the overall quality of aluminum alloy die-cast specimens, aiming to provide a reference for related research.
Specimen size is 300 mm * 300 mm, and thickness is 3 mm. Casting process design and sampling locations for test specimens are shown in Figure 1, where locations 1-6 are sampling points. A 3500 kN Toyo horizontal cold chamber die-casting machine was used for specimen preparation. Chamber diameter was 50 mm, effective chamber length was 370 mm, and designed filling degree was 38.5%. To verify results, tensile tests were conducted at six different locations on test specimens. Specimens met requirements for Type B tensile specimens in non-ferrous metal die casting as specified in GB/T13822-2017, as shown in Figure 2.
Tests used AlSi10MnMg (AC-43500, EN 1706), a commonly used material for structural components. Its main components and mechanical property requirements are shown in Tables 1 and 2.
die-casting process 
Figure 1. Casting structure and sampling location of die-cast specimen
die-casting process 
Figure 2. Schematic diagram of dimensions of type B tensile specimens according to GB T13822-2017
die-casting process 
Table 1. Main chemical composition (%) of AlSi10MnMg alloy
Tensile strength/MPa Yield strength/MPa Elongation/%
250 120 5
Table 2. Mechanical properties of as-cast AlSi10MnMg alloy
Based on specimen wall thickness, chamber filling degree, and simulation results, process parameters adopted for T1 test are shown in Table 3.
Specimens produced using above process have qualified appearance and internal quality, as shown in Figures 3 and 4. Three specimens were cut into tensile specimens at positions shown in Figure 1, and tensile test results are shown in Table 4. Figure 4 shows that fracture surface of specimens contains foreign matter, with a proportion as high as 61%.
In tensile test, foreign matter on specimen fracture surface appears as bright, flaky areas, which is inconsistent with rough, matte morphology of a normal fracture surface. Tensile strength, yield strength, and elongation of specimens with foreign matter are all lower than normal levels, indicating that foreign matter has a significant impact on mechanical properties of specimens.
Injection pressure p/MPa Fast injection speed v1/(m.s-1) Fast injection transition position S1/mm Pressure boosting position S2/mm
90~100 2.5 240 320
Slow injection speed v2/(m.s-1) Aluminum material temperature T1/℃ Fixed mold temperature T2/℃ Moving mold temperature T3/℃
0.1~0.2 665~670 115-120 115-120
Table 3 T1 Specimen Parameters
die-casting process 
Figure 3 Specimen Quality Qualified
die-casting process 
Figure 4 Comparison of Fracture Surface Appearance
die-casting process 
Table 4 Mechanical Properties of Specimens
Fracture surfaces of foreign objects all exhibited varying degrees of flaky, bright fracture surfaces, which are significantly different from irregularly shaped, rough, matte fracture surfaces of normal fracture surfaces (see Figure 4).
Scanning electron microscopy (SEM) analysis was performed on abnormal fracture surfaces, normal fracture surfaces, fracture surfaces containing impurities (see Figure 5). It can be seen that bright fracture surfaces of foreign object fracture surfaces (Figure 5a) and normal fracture surfaces (Figure 5b) primarily contain Al, Si, and Mg alloying elements. This differs from fracture surfaces caused by general impurities (Figure 5c), which contain C and O compounds. Therefore, bright fracture surfaces of abnormal fracture surfaces are not caused by impurities. Furthermore, Si content in bright areas is significantly higher than material composition indicated. This region is rich in Si, which can be attributed to segregation caused by unbalanced solidification.
Metallographic structure of foreign object fracture surface is mainly divided into four regions, as shown in Figure 6. Region 1 contains normal primary Al phase and Al-Si eutectic structure. Region 2, with a small area, is a transitional region between Region 1 and Region 3, where Al-Si eutectic structure begins to decompose, and Si particles appear. Region 3, with a large area, shows disappearance of Al-Si eutectic structure, leaving only Al and Si phases. Al phase remains dendritic, a typical characteristic of cold material. In Region 4, Al phase no longer exhibits a dendritic state, fine silicon particles are evenly and densely distributed. Metallographic analysis shows that location of abnormal fracture surface is consistent with typical characteristics of cold material, and it can be determined that it is caused by inclusion of pre-solidified aluminum material during casting process. Metallographic structure of normal tensile fracture surface shows a relatively uniform and smooth Al-Si eutectic distribution, as shown in Figure 7.
die-casting process 
Figure 5 Scanning electron microscopy analysis of fracture surface
die-casting process 
Figure 6 Schematic diagram of metallographic structure and zoning of foreign object fracture surface
die-casting process 
Figure 7 Metallographic structure of normal fracture surface
Insufficient melting can lead to retention of solid metal particles. Because this study adopted an external direct supply of molten aluminum, had strict requirements for temperature, refining, and testing processes of molten aluminum arriving at factory, problem of insufficient melting was eliminated. Specific quality control measures for molten aluminum are as follows: ① Temperature control: Temperature of AlSi10MnMg molten aluminum arriving at factory must be controlled between 710 and 730 ℃. ② Refining process: After molten aluminum arrives at factory, it must undergo argon refining for at least 15 minutes. ③ Testing process: After refining, molten aluminum must undergo 100% K-mold testing and density testing to confirm its quality is up to standard. ④ Temperature testing: Temperature must be tested again before pouring to ensure it meets requirements. ⑤ Holding furnace temperature: Temperature of holding furnace at machine side is controlled between 665 and 670 ℃.
Design of mold cooling channels and gating system directly affects flow and temperature distribution of alloy molten aluminum. This test piece is a simple flat plate product with uniform wall thickness; therefore, mold cooling channels adopt a uniform distribution design (see Figure 8), and are equipped with a mold temperature controller for precise temperature control. Figure 9 shows a simulation of filling process. Gating system was verified through simulation analysis. Molten aluminum filled cavity smoothly and sequentially throughout filling process, indicating that gating system design was reasonable.
die-casting process 
Figure 8 Distribution of water pipes in mold
die-casting process 
Figure 9 Filling simulation analysis
Low temperature during die casting is one of main causes of cold material defects. Specifically, this includes low molten aluminum pouring temperature, low mold temperature, and low barrel temperature.
(1) Low molten aluminum pouring temperature
For die-cast aluminum alloys, when Si content is in the range of 5%~18%, the higher Si content, the better fluidity of molten aluminum; while the higher Mg content, the worse fluidity. AlSi10MnMg alloy used in this experiment has a Si content of 9.0%~11.5% and a Mg content of 0.40%~0.45%. Figure 10 shows effect of alloying elements on fluidity of die-cast alloy liquid. It can be seen that fluidity of this material is relatively poor, and it is easy to entangle cold material during filling process. This fluidity characteristic is determined by characteristics of elements in material. To reduce risk of cold material, temperature of molten aluminum can be appropriately increased to ensure sufficient fluidity when filling mold cavity. Experiment increased furnace temperature from (670±5) ℃ to (690±5) ℃ and (710±5) ℃ respectively for production testing. Tensile data from test pieces showed that fracture ratio of cold material characteristics was 55% at (690±5) ℃, with no significant improvement; while at (710±5) ℃, fracture ratio was 19%, showing a significant improvement.
die-casting process 
Figure 10 Influence of alloying elements on fluidity of die-casting alloy liquid
(2) Too low mold temperature
When mold temperature is too low, molten alloy will solidify rapidly after entering mold cavity, forming cold material, which will be drawn into casting. According to experimental data, a mold cavity surface temperature of 115~120 ℃ is significantly too low. In actual production, mold cavity surface temperature should usually be controlled between 150~230 ℃. Therefore, it is necessary to adjust mold temperature controller to raise surface temperature of mold cavity to above 150 ℃ to ensure stability of production process.
(3) Low Barrel Temperature
When molten metal is poured into barrel, aluminum molten metal at the front end that is in contact with barrel will quickly solidify at the bottom of sleeve, forming a layer of aluminum sheet. As punch moves forward, aluminum sheet is broken into small pieces (sheet-like cold material), pushed into runner and casting. Because these pre-solidified aluminum sheet fragments come into contact with lubricants (such as punch oil, mold release agent, etc.), their contact surfaces will form a bright, smooth surface. This surface will not adhere to other aluminum materials, but will instead form cracks, which may lead to leakage or become starting point of breakage. Since temperature difference between barrel and molten aluminum is unavoidable, front end cold material fragments cannot be completely eliminated, but this impact can be minimized through process management measures. Following measures were taken for this test mold.
Measure 1: Adjust mold temperature controller parameters to raise barrel temperature from 150 ℃ to 180 ℃. During die casting, theoretical temperature inside pressure chamber should be above 350 ℃. Since actual temperature inside pressure chamber could not be directly measured in this experiment, temperature was obtained by measuring a fixed point on outer side of barrel front using an infrared thermometer.
Measure 2: Wrap barrel with an insulating blanket to reduce heat loss and ensure stable barrel temperature during die casting (see Figure 11).
die-casting process 
Figure 11 Insulating blanket wrapped around barrel
Inappropriate injection parameters may cause molten aluminum to remain in barrel for too long, forming a surface solidification layer. Adjusting injection parameters to increase filling speed and shorten residence time of molten aluminum can effectively reduce cold material defects. Optimized parameters are shown in Table 5.
Using a conventional open-type electric holding furnace, surface of molten aluminum is exposed to air for a long time, easily forming an alumina film which is introduced during material handling. To address this, scoop structure was optimized (see Figure 12), smelting workers are required to regularly observe surface of molten aluminum and clean off any slag to avoid introducing surface aluminum film into barrel, thus reducing cold material defects.
Injection pressure p/MPa Fast injection speed v1/(m.s-1) Fast injection transition position S1/mm Pressure boosting position S2/mm
90~100 2.8 240 340
Slow injection speed U2/(m.s-1) Aluminum material temperature T1/℃ Fixed mold temperature T2/℃ Moving mold temperature T3/℃
0.3~0.5 700~710 150 150
Table 5 Optimized Parameters
die-casting process 
Figure 12 Optimized Spoon Structure
Above optimization measures were implemented, optimized process parameters were adopted. Specimens were cut and tensile tested, and results are shown in Table 6. Observation shows that cold material defects inside aluminum alloy die-cast specimens were significantly reduced, proportion of abnormal fracture surfaces decreased from 61% to 11%, mechanical properties of specimens were significantly improved, meeting material performance requirements.
Comparative analysis of fracture surfaces and their metallographic structure revealed that area of cold material region was also significantly reduced, as shown in Figure 13.
die-casting process 
Table 6 Optimized Specimen Tensile Data
die-casting process 
Figure 13 Cold Material Fracture Surface Appearance and Metallographic Analysis
Conclusion
Through systematic experimental analysis, formation mechanism of cold material defects inside aluminum alloy die-cast specimens was explored in depth, and a series of optimization measures were proposed. Increasing temperature of die-casting process, especially temperature of molten aluminum, significantly improved cold material defects in material specimens, but defect rate was still close to 20%. Simultaneously, comprehensive implementation of above measures can effectively reduce cold material defect rate and improve quality of specimens.

Go To Top