Polishing: A Key Step in Injection Mold Making

Time:2026-11-10 08:59:28 / Popularity: / Source:

Anyone in mold-making industry knows that polishing is incredibly important. It's no less crucial than initial machining; it's the most critical process in mold manufacturing, significantly impacting many aspects. 
Appearance of plastic part, its dimensional accuracy, smoothness of demolding, and even mold's lifespan all depend on quality of the polishing. This is no exaggeration. Proper polishing allows you to achieve mirror-like high gloss, delicate matte finishes, and various special textures. Furthermore, it improves mold's wear resistance and corrosion resistance, significantly reducing defects in plastic parts. Furthermore, smoothness of demolding directly affects production efficiency and yield rate. Polishing, while considered a technical skill, is more of a craft. Experience and a feel for work are paramount. Same job done by different craftsmen yields vastly different results.
Injection Mold Making 

I. Common Types of Mold Surface Treatments

These are commonly used: oilstone polishing, sandpaper polishing, and mirror polishing.
1. Oilstone Polishing
This is the most basic polishing level, primarily used to remove obvious machining marks from mold surface. Yes, it removes tool marks. Texture isn't very regular. It's fine for general consumer products, but definitely not suitable for high-precision products. Oilstones also come in various grit grades; choose the one that suits your needs.
2. Sandpaper Polishing
This produces a smoother finish and higher gloss than oilstone polishing. When sanding, you must work in one direction only. Result is a fine, matte finish. And, to achieve a mirror finish, you must first go through sandpaper polishing; it's unavoidable. Also, don't underestimate difference in gloss from sandpaper polishing. Even a slight difference can result in either a high-end matte finish or a cheap, plasticky look—it's very noticeable.
3. Mirror Polishing
Surface is extremely bright, almost completely smooth, resulting in a glossy, slippery finish on mold. Suitable for high-precision, low-friction industrial parts, but this is too time-consuming and costly. Unless absolutely necessary, it's really unnecessary and not worthwhile.
By the way, smoothness of mold surface is crucial for demolding. Seriously, whether it's too rough or too smooth, it's no good; both will cause problems. If surface is too rough, even rougher than an oilstone surface, friction will be enormous, making demolding extremely difficult and prone to scratching plastic parts—a huge hassle. If it's too smooth, like a mirror finish, it's prone to sticking to mold. If plastic parts stick to mold, ejector pins will break it, delaying production and lengthening production cycle. Therefore, don't aim for an excessively high finish. Just achieve minimum required smoothness to ensure both appearance and functionality, and smooth demolding—that's the best approach.

II. Polishing equipment, tools, and consumables

These must all be readily available; don't compromise.
1. Equipment
A handheld flexible shaft polisher is essential, along with a foot pedal speed control, a right-angle head, a reciprocating polishing head, and a straight-handled polishing pen. For deep cavities and narrow crevices that are difficult to reach by hand, specialized attachments are necessary; otherwise, polishing is impossible.
2. Consumables
Oilstones are available in 180#, 300#, 400#, and 600# grits, as well as 2602 and 1602 models; all must be on hand. Wet sandpaper is available in 600# and 1200# grits. Diamond polishing paste is available in yellow (6μm), green (3μm), and blue (1μm); these three are commonly used. Also needed are cup brushes, end-face brushes, wheel brushes, and felt polishing heads. Protective steel plates are also necessary to protect sharp corners and edges, otherwise, they may easily break during polishing.
Important points for equipment use: Specialized tools must be used; do not use other equipment as a makeshift solution. Quality of your tools directly impacts polishing quality and efficiency, and a mold factory's competitiveness hinges entirely on this. For complex mirror finishes or difficult-to-work cavities, don't try to do it yourself; outsourcing to a professional polishing factory is much more reliable.

III. Polishing Standards:

Grade A is diamond polishing. A-1 uses #3 diamond, achieving a mirror finish with Ra 0.012-0.025; A-2 uses #6 diamond, achieving high gloss with Ra 0.025-0.05; A-3 uses #15 diamond, achieving high gloss with Ra 0.05-0.10.
Grade B is sandpaper polishing. B-1 uses 600# sandpaper, achieving a medium-high gloss with Ra 0.05-0.10; B-2 uses 400# sandpaper, achieving a medium gloss with Ra 0.10-0.15; B-3 uses 320# sandpaper, achieving a medium-low gloss with Ra 0.28-0.32.
Grade C is for oilstone polishing: C-1600# oilstone, low gloss, Ra 0.35-0.40; C-2400# oilstone, low gloss, Ra 0.45-0.55; C-3320# oilstone, low gloss, Ra 0.63-0.70.
Grade D is for dry blasting: D-1 glass beads, satin finish, Ra 0.80-1.00; D-2# 240 alumina, matte finish, Ra 1.00-2.80; D-3# 24 alumina, coarse matte finish, Ra 3.20-18.0.
Furthermore, compatibility of different grades varies for plastics such as ABS, PP, PS, HDPE, nylon, PC, TPU, and acrylic. This should also be noted.

IV. Polishing Methods

Mechanical Polishing: Mostly done manually, using oilstones, sandpaper, and rough wheels to cut or level surface. Low cost, the most common method, achieving a Ra of up to 0.008μm, quite impressive.
Chemical Polishing: Uses chemical solvents to dissolve small protrusions on the surface. Suitable for complex-shaped molds, and can process several at once, offering high efficiency.
Electrolytic Polishing: Similar to chemical polishing, but uses electric current to dissolve protrusions. Divided into macroscopic leveling and microscopic leveling, offering more stable results and achieving Ra less than 1μm.
Ultrasonic Polishing: Using abrasive suspension combined with ultrasonic vibration. Used for microstructures and complex cavities, minimizing workpiece deformation.
Fluid Polishing: Also called hydro-grinding, using high-speed fluid carrying abrasive particles to polish the surface. Most suitable for internal channels, deep cavities, and complex cavities.
Magnetorheological polishing: also known as magnetorheological abrasive polishing, uses an abrasive brush formed within a magnetic field for polishing. It is highly efficient and offers good precision control, achieving a Ra of 0.1μm.

V. Standard ten-step polishing method

This is a practical method that must be followed step-by-step; none of steps can be skipped.
Remove EDM work-hardened layer with a 320# oilstone - Use a soft-bonded oilstone to remove surface pits - Switch to a 2602 oilstone and polish alternately - Use a 1602 oilstone for fine finishing - Use 600# wet sandpaper to remove oilstone marks - Use 6μm diamond polishing paste with a brush to remove sandpaper marks - Use a felt wheel to remove brush marks - Use a 3μm green diamond polishing wheel for fine finishing - Use a hand felt wheel for a final, meticulous finish - Finally, use a tissue dampened with green diamond polishing wheel for manual finishing.

VI. Polishing Principles

The entire process must be clean, extremely clean. Coarse particles mixed in will leave scratches on the surface, rendering the work useless. Never skip grits when polishing. You must proceed from coarse to fine, step by step according to grit size. Skipping grades will definitely cause problems. Don't apply too much pressure. Too much pressure will result in orange peel texture, ruining the entire surface. Protective steel sheets must be used to clamp edges and corners; otherwise, edges will be polished unevenly and corners may collapse.

VII. Polishing Precautions

Before polishing, make sure to discuss everything clearly with polishing technician and write it down. Don't just talk about it verbally, or you'll easily make mistakes.
Mark all surfaces that meet polishing test with a marker; Clearly state and mark which sharp corners and edges must be kept sharp; Specify in advance which corners need to be rounded before polishing; Specify area where texture will be applied, its type, and depth, for example, 0.015 mm, 0.030 mm. Write everything clearly; What type of steel is used for mold cavity? What is its hardness? This must be specified; Do venting channels and venting grooves need polishing? Are there any machining allowances? Confirm this; Are contact surfaces properly machined? Is mold assembly complete? Is adhesive protection needed? What final surface finish grade is required? Specify this clearly; How was workpiece machined? Was it heat-treated? Was it CNC-machined with carbide cutting tools? This is very important; High-grade mirror finishes may require stress relief. Carbide cutting creates a hardened layer, making polishing more difficult. An acid etching test must be performed before texturing. EDM-machined surfaces must be tested; Which inserts should be polished first, and which should have machining allowances? Avoid rounding them. Plan everything clearly.
Injection Mold Making 
Also, some precautions for on-site work; there are so many pitfalls to avoid.
Be extremely careful if you've already used a 320# oilstone for rough polishing. This level will cover up many small defects. They might look fine initially, but after fine polishing, they'll all be visible, requiring you to return to 220# for re-grinding – a huge hassle. Also, consider whether to do it in-house or outsource. For simple surfaces, in-house polishing is fine. For mirror finishes, complex cavities, or high-requirement work, find a professional outsourcing factory. Don't try to save money on this.
Professional polishing factories process ten times more molds a year than ordinary workshops. They have more experience, saving you time and reducing errors. There are also important points to consider when handing over molds. Make a list of all parts and inserts to be polished to avoid losing anything. All requirements must be written down for written confirmation. Don't just rely on verbal agreements; otherwise, you'll have no evidence for future disputes. Deliver mold on time and retrieve it promptly after polishing. Before handing over, thoroughly clean cavities and cores with an air gun to remove any metal shavings or impurities.

VIII. Common Polishing Problems

Orange peel texture is mostly caused by incorrect polishing pressure, uneven steel structure, or localized overheating; Pockmarks and pinholes are caused by impurities or inclusions in steel itself, or abrasive particles embedded in the surface; Mold sticking is either due to an overly smooth mirror finish, lack of draft angle, or excessively strong plastic adhesion.
Different steels have different polishing difficulties. H13 steel is relatively easier to polish, while 420 stainless steel is much more difficult and requires a finer oilstone. Furthermore, different engineering plastics can exhibit significant differences in appearance, mold release, and adhesion even at the same surface finish, especially around ribs and on surfaces without draft angles. It is crucial to select polishing grade based on plastic material.