Injection Molding Defect Quick Reference Handbook: Shrinkage, Deformation, Flash... One diagram help
Time:2026-11-09 16:37:33 / Popularity: / Source:
Target Audience: Structural Engineers, Injection Molding Engineers, SQEs, NPIs.
Applicable Scenarios: Mold trial problem recording, mass production anomaly analysis, supplier communication.
Core Viewpoint: Defect analysis should first define phenomenon, then look at location and pattern, and finally determine whether it's a material, mold, process, or structural issue.
T0 The Most Common Scenario at Mold Trial Site
"Mr. Wang, come take a look, this part has shrunk." You go over and see, it has indeed shrunk. Then what?
Increase holding pressure? Shrinkage might be reduced, but deformation will be more severe after high temperature. Lower mold temperature? Shrinkage is slightly improved, but weld lines appear. Change structure? Mold is already made, it can't be changed. Where is problem? Lack of a systematic defect analysis framework.
This article is to help you build this framework. Next time you encounter a problem during a mold trial, check in this order to save yourself three days of wasted time.
1. Basic Methods of Defect Analysis
Define defect phenomena → Record location and frequency → Confirm mold cavity/ machine/ batch → Compare with process parameters → Determine material/ mold/ process/ structure → Verify with a small DOE → Confirm improvement measures.
Don't just write "Appearance Defect" or "Deformation," you must record: Defect Photo; Location of Occurrence; Defect Direction; Mold Number, Cavity Number; Material Batch; Process Parameters; Did it occur after high temperature?
Applicable Scenarios: Mold trial problem recording, mass production anomaly analysis, supplier communication.
Core Viewpoint: Defect analysis should first define phenomenon, then look at location and pattern, and finally determine whether it's a material, mold, process, or structural issue.
T0 The Most Common Scenario at Mold Trial Site
"Mr. Wang, come take a look, this part has shrunk." You go over and see, it has indeed shrunk. Then what?
Increase holding pressure? Shrinkage might be reduced, but deformation will be more severe after high temperature. Lower mold temperature? Shrinkage is slightly improved, but weld lines appear. Change structure? Mold is already made, it can't be changed. Where is problem? Lack of a systematic defect analysis framework.
This article is to help you build this framework. Next time you encounter a problem during a mold trial, check in this order to save yourself three days of wasted time.
1. Basic Methods of Defect Analysis
Define defect phenomena → Record location and frequency → Confirm mold cavity/ machine/ batch → Compare with process parameters → Determine material/ mold/ process/ structure → Verify with a small DOE → Confirm improvement measures.
Don't just write "Appearance Defect" or "Deformation," you must record: Defect Photo; Location of Occurrence; Defect Direction; Mold Number, Cavity Number; Material Batch; Process Parameters; Did it occur after high temperature?
2. Quick Check of Common Defects
| Defect | Manifestation | Common Causes | Priority Check |
| Shrinkage | Surface depressions | Thick material, insufficient holding pressure, slow cooling | Structural thickness, holding pressure, cooling |
| Deformation | Warping, twisting | Uneven shrinkage, uneven cooling, stress release | Measurement benchmark, cooling, gate |
| Short shot | Incomplete filling | Insufficient flow, poor venting, insufficient pressure | Material temperature, speed, gate, venting |
| Flash | Parting line overflow | Insufficient clamping, high pressure, mold clearance | Clamping force, holding pressure, mold wear |
| Weld line | Merging line of two material flows | Low material temperature, poor venting, unreasonable gate | Material temperature, mold temperature, venting |
| Silver streaks | Silver streaks on the surface | Moisture, volatiles, shearing | Drying, back pressure, material temperature |
| Air streaks | Flow marks | Poor venting, improper speed | Ventilation, speed, gate |
| Burning | Local blackening | Trapped air compression and heating | End venting, injection speed |
| Whitening | Whitening at ejection point | High ejection force, insufficient draft angle | Ejection area, polishing, draft angle |
| Flow marks | Surface flow lines | Low material temperature, small gate, unstable speed | Material temperature, mold temperature, gate |
3. Shrinkage
Shrinkage often occurs at: Back of pillars; Back of thick ribs; Thick-walled corners; Far end of gate; Local thick areas of plastic on large flat surfaces.
Shrinkage often occurs at: Back of pillars; Back of thick ribs; Thick-walled corners; Far end of gate; Local thick areas of plastic on large flat surfaces.
Priority troubleshooting order: Is there localized thick plastic? Is holding pressure properly transmitted? Is gate freezing prematurely? Is cooling insufficient? Is material shrinkage rate too high?
A common misconception: Increase holding pressure for shrinkage. However, if shrinkage originates from thicker plastic material itself, increasing holding pressure will only increase internal stress, leading to more severe deformation at high temperatures. First, examine structure, then adjust process.
4. Weld Lines
Weld lines are not only an aesthetic issue but can also be a strength problem.
A common misconception: Increase holding pressure for shrinkage. However, if shrinkage originates from thicker plastic material itself, increasing holding pressure will only increase internal stress, leading to more severe deformation at high temperatures. First, examine structure, then adjust process.
4. Weld Lines
Weld lines are not only an aesthetic issue but can also be a strength problem.
High-risk locations: Root of snap fastener; Around screw post; Drop stress zone; Transparent parts; Sealing surface.
Improvement directions: Adjust gate position; Increase material/mold temperature; Improve venting; Add overflow wells; Prevent weld lines from falling into stress zones.
How much does strength of weld lines affect? For same material, impact strength at a weld line location may only be 30-50% of that at a non-weld line location. Location of weld lines must be considered when designing snap fasteners.
5. Flash
Flash may originate from: Excessive holding pressure; Injection speed too fast; Insufficient clamping force; Parting surface wear; Ventilation groove too deep; Mold not adapted after high-flow-rate material change.
Improvement directions: Adjust gate position; Increase material/mold temperature; Improve venting; Add overflow wells; Prevent weld lines from falling into stress zones.
How much does strength of weld lines affect? For same material, impact strength at a weld line location may only be 30-50% of that at a non-weld line location. Location of weld lines must be considered when designing snap fasteners.
5. Flash
Flash may originate from: Excessive holding pressure; Injection speed too fast; Insufficient clamping force; Parting surface wear; Ventilation groove too deep; Mold not adapted after high-flow-rate material change.
Flash cannot be solved by simply reducing pressure. If reducing pressure leads to shrinkage or short shots, it indicates that mold closure, venting, or material matching also need to be checked.
6. Ejector whitening and cracking
Ejector whitening of PP parts is commonly caused by: Ejector pin area too small; Uneven ejection; Insufficient draft angle; Excessively deep surface texture; Excessive holding pressure causing mold sticking.
Improvement directions: Increase ejection area; Adjust ejector pin position; Increase draft angle; Reduce local holding pressure stress; Check mold polishing and texture direction.
7. Special Attention for Large PP Parts
Large PP parts are most prone to following combinations: Shrinkage; + Deformation; + Warping after high temperatures; + Increased assembly gaps; + Cracked screw posts or clips.
Don't look at these defects in isolation. It's recommended to overlay defect locations onto same image to see if they correspond: Thick glue areas; Far from gate; Cooling blind areas; Dense rib areas; Strong assembly constraint points.
8. Determine cause by "location"
Defect location is usually more important than defect name.
6. Ejector whitening and cracking
Ejector whitening of PP parts is commonly caused by: Ejector pin area too small; Uneven ejection; Insufficient draft angle; Excessively deep surface texture; Excessive holding pressure causing mold sticking.
Improvement directions: Increase ejection area; Adjust ejector pin position; Increase draft angle; Reduce local holding pressure stress; Check mold polishing and texture direction.
7. Special Attention for Large PP Parts
Large PP parts are most prone to following combinations: Shrinkage; + Deformation; + Warping after high temperatures; + Increased assembly gaps; + Cracked screw posts or clips.
Don't look at these defects in isolation. It's recommended to overlay defect locations onto same image to see if they correspond: Thick glue areas; Far from gate; Cooling blind areas; Dense rib areas; Strong assembly constraint points.
8. Determine cause by "location"
Defect location is usually more important than defect name.
| Defect Locations | Prior Suspicion |
| Near gate | Excessive shear, excessive holding pressure, insufficient gate cooling. |
| At the end of flow | Insufficient venting, short shots, insufficient holding pressure transfer. |
| On the back of thick plastic | Shrinkage, voids, insufficient cooling. |
| Near weld line | Venting, material temperature, mold temperature, gate location. |
| Ejector pin location | Ejection force, draft angle, mold clamping. |
| Parting surface | Flash, clamping force, mold wear. |
| Snap-in/Pillar positions | Stress concentration, material toughness, excessive holding pressure. |
| Center of large flat surfaces | Uneven cooling, rib stretching, insufficient rigidity. |
A rule of thumb: If defects consistently appear in fixed locations, prioritize checking structure and mold; if defect locations are random, prioritize checking material, process, operational stability.
9. Determine cause based on "time"
9. Determine cause based on "time"
| Time of Occurrence | Most Likely Cause |
| Immediately after demolding | Directly caused by structure, mold, or process |
| Becomes more noticeable after 24 hours | Post-shrinkage, residual stress release |
| Appears only after high temperature | Heat resistance, stress release, assembly constraints |
| Appears only after drop | Material toughness, weld lines, notch stress |
| Appears after a period of mass production | Mold wear, water channel blockage, material batch changes |
| Appears after shift change | Differences in operation, machine, and parameter execution |
This judgment is very important. For example, "OK at room temperature, warping after high temperature" cannot be simply treated as deformation immediately after demolding.
10. Determine cause by "Cavity/Machine/Batch"
10. Determine cause by "Cavity/Machine/Batch"
| Phenomenon | More Likely Cause |
| Only one cavity is abnormal | Local cavity cooling, venting, ejection, or dimensional issues |
| Anomalous in same direction for all cavities | Structural design, gate scheme, material shrinkage |
| Anomalous on a specific machine | Machine precision, mold clamping, temperature control, screw status |
| Anomalous on a specific shift | Operational consistency, parameter execution, material drying |
| Anomalous on a specific batch of materials | Material batch, masterbatch, recycled material ratio |
| Anomalous after weather changes | Raw material moisture content, workshop temperature and humidity, cooling water temperature |
During on-site troubleshooting, it is recommended to perform cross-validation first: Change machine with same material; Change material on same machine; Compare cavities when changing molds with same mold; Observe continuous production with same parameters.
11. Defect Retrospective Template
For each trial molding or mass production anomaly, it is recommended to record it using a unified template:
11. Defect Retrospective Template
For each trial molding or mass production anomaly, it is recommended to record it using a unified template:
| Item | Record Content |
| Defect Name | Shrinkage, Deformation, Flash, Weld Lines, etc. |
| Defect Photo | Mark Location and Direction |
| Part Information | Part Number, Version, Mold Number, Mold Cavity |
| Material Information | Grade, Batch, Masterbatch, Recycled Material Ratio |
| Process Parameters | Material Temperature, Mold Temperature, Speed, Holding Pressure, Cooling |
| Occurrence Conditions | Immediately after demolding, 24 hours later, after high temperature, after drop |
| Measurement Data | Dimensions, Flatness, Weight, Assembly Clearance |
| Preliminary Cause Attribution | Material/Structure/Mold/Process/Assembly |
| Improvement Measures | Parameter Adjustment, Mold Repair, Structure Modification, Material Change |
| Effect Evaluation | Whether to Close, Any Side Effects |
Without a retrospective template, trial molding experience is difficult to accumulate, and you will likely repeat same mistakes next time.