Solving "Internal Damage" Problem of Motor Housings: Rotary Casting + Precision Heat Treat
Time:2026-11-23 09:58:58 / Popularity: / Source:
New energy vehicles are main direction for transformation and upgrading of global automotive industry and green development, and also a strategic choice for high-quality development of China's automotive industry. With annual increase in production and sales of new energy vehicles, electric drive industry has developed rapidly, and demand for motor housings, as key components, has also increased accordingly. Current development of new energy motor housings is characterized by rapid growth and technological innovation. In terms of industrial chain and core technologies, quality and performance of new energy motor housings, as one of core components of new energy vehicles, directly affect power, climbing ability, and acceleration performance of the entire vehicle.
Main cooling methods for new energy drive motors are water cooling and oil cooling. Water-cooled motors have advantages in energy saving and cost reduction. New energy water-cooled motor housings have efficient, reliable, and stable thermal management functions. Water-cooled motor housing adopts a sandwich structure with spiral water channels within sandwich layer. Through connection of inlet and outlet water pipes, efficient water circulation cooling is achieved, significantly improving motor's heat dissipation. Furthermore, water-cooled motor housing design is lightweight, employing friction stir welding technology to further reduce the overall weight of vehicle, facilitating transportation and installation. This design not only helps improve motor operating efficiency but also extends motor's service life. Water-cooled motor housings typically utilize efficient cooling systems and precision manufacturing processes to ensure excellent performance even in high-temperature environments.
Water-cooled motor housing is made of A380 die-cast aluminum alloy, consisting of an outer shell and an inner shell. A series of processes, including vertical lathe operation, T5 heat treatment, hot fitting, friction stir welding, and post-weld assembly machining, are used to form a sealed water-cooled cavity motor housing. Failure modes of motor inner shell casting are numerous, including internal non-density failure, crack failure, wear failure, corrosion failure, and deformation failure. These failure modes are result of multiple factors, potentially including material properties, design and manufacturing processes, and operating conditions. The most significant failure mode of water-cooled motor inner housing in this study was internal density failure. Internal density failure of motor inner housing casting leads to a decline in its mechanical properties, making it prone to leakage, cracking, and deformation during use, thus affecting product's service life and safety. Slight internal density failure can cause coolant leakage, affecting motor efficiency; severe internal density failure may lead to inner housing rupture, affecting normal motor operation.
Factors affecting internal density failure of motor inner housing casting include composition and melting process of die-cast aluminum alloy, design of die-casting gating system, die-casting process parameters, T5 heat treatment process, hot-fitting press-fitting process, and friction stir welding process. This study, with die-cast aluminum alloy composition, melting process, and die-casting process parameters fixed, focuses on four modules: gating system, T5 heat treatment process, hot-fitting press-fitting process, and friction stir welding process, exploring their impact on performance of motor inner housing.
Motor inner housing has a cylindrical structure. The entire product falls within leak-testing and sealing area, therefore, requirement for its internal density is extremely high. To ensure high density and compactness of motor's inner casing, casting gating system design must be highly rational. By rationally designing location, shape, size of ingate, and ensuring smooth molten metal flow, internal density of die-cast part can be effectively guaranteed. In the early stages of development, based on motor's inner casing structure and performance requirements, suitable gating locations were identified, and four different gating systems were pre-designed (see Figure 1). Scheme 1 uses a beak-type single-sided gating system; Scheme 2 uses a flat-overlapping center gating system; Scheme 3 uses a flat-overlapping single-sided gating system; Scheme 4 uses a beak-type center gating system.
Mold flow analysis of four different gating schemes was performed using Magma software (see Figure 2). Option 1 uses a beak-type gate, but when aluminum melt has filled mold cavity, a significant amount of gas remains on sidewalls of casting, posing a risk of trapped and entangled gas. Option 2 uses a center gate, where aluminum enters mold cavity from center of inner shell. This results in uniform gate distribution, consistent aluminum filling, smooth flow, and no turbulence or entrapment, allowing for smooth gas escape and minimizing risk of porosity. Option 3 uses a flat-bottom gate, but due to depth of inner shell cavity, filling is not smooth, leading to a high gas content on sidewalls after filling. Option 4 uses a beak-type gate, pouring onto sidewalls of inner shell. While filling is smooth, severe entrapment and entrapment occur, causing rapid temperature drop at entrapment site and posing a significant risk of poor forming and exposed porosity. Therefore, based on mold flow results, Option 2 (flat-bottom center gate) was ultimately chosen for motor inner shell gating system, with gate located on the wall of machined hole at the bottom of inner shell cylinder.
Main cooling methods for new energy drive motors are water cooling and oil cooling. Water-cooled motors have advantages in energy saving and cost reduction. New energy water-cooled motor housings have efficient, reliable, and stable thermal management functions. Water-cooled motor housing adopts a sandwich structure with spiral water channels within sandwich layer. Through connection of inlet and outlet water pipes, efficient water circulation cooling is achieved, significantly improving motor's heat dissipation. Furthermore, water-cooled motor housing design is lightweight, employing friction stir welding technology to further reduce the overall weight of vehicle, facilitating transportation and installation. This design not only helps improve motor operating efficiency but also extends motor's service life. Water-cooled motor housings typically utilize efficient cooling systems and precision manufacturing processes to ensure excellent performance even in high-temperature environments.
Water-cooled motor housing is made of A380 die-cast aluminum alloy, consisting of an outer shell and an inner shell. A series of processes, including vertical lathe operation, T5 heat treatment, hot fitting, friction stir welding, and post-weld assembly machining, are used to form a sealed water-cooled cavity motor housing. Failure modes of motor inner shell casting are numerous, including internal non-density failure, crack failure, wear failure, corrosion failure, and deformation failure. These failure modes are result of multiple factors, potentially including material properties, design and manufacturing processes, and operating conditions. The most significant failure mode of water-cooled motor inner housing in this study was internal density failure. Internal density failure of motor inner housing casting leads to a decline in its mechanical properties, making it prone to leakage, cracking, and deformation during use, thus affecting product's service life and safety. Slight internal density failure can cause coolant leakage, affecting motor efficiency; severe internal density failure may lead to inner housing rupture, affecting normal motor operation.
Factors affecting internal density failure of motor inner housing casting include composition and melting process of die-cast aluminum alloy, design of die-casting gating system, die-casting process parameters, T5 heat treatment process, hot-fitting press-fitting process, and friction stir welding process. This study, with die-cast aluminum alloy composition, melting process, and die-casting process parameters fixed, focuses on four modules: gating system, T5 heat treatment process, hot-fitting press-fitting process, and friction stir welding process, exploring their impact on performance of motor inner housing.
Motor inner housing has a cylindrical structure. The entire product falls within leak-testing and sealing area, therefore, requirement for its internal density is extremely high. To ensure high density and compactness of motor's inner casing, casting gating system design must be highly rational. By rationally designing location, shape, size of ingate, and ensuring smooth molten metal flow, internal density of die-cast part can be effectively guaranteed. In the early stages of development, based on motor's inner casing structure and performance requirements, suitable gating locations were identified, and four different gating systems were pre-designed (see Figure 1). Scheme 1 uses a beak-type single-sided gating system; Scheme 2 uses a flat-overlapping center gating system; Scheme 3 uses a flat-overlapping single-sided gating system; Scheme 4 uses a beak-type center gating system.
Mold flow analysis of four different gating schemes was performed using Magma software (see Figure 2). Option 1 uses a beak-type gate, but when aluminum melt has filled mold cavity, a significant amount of gas remains on sidewalls of casting, posing a risk of trapped and entangled gas. Option 2 uses a center gate, where aluminum enters mold cavity from center of inner shell. This results in uniform gate distribution, consistent aluminum filling, smooth flow, and no turbulence or entrapment, allowing for smooth gas escape and minimizing risk of porosity. Option 3 uses a flat-bottom gate, but due to depth of inner shell cavity, filling is not smooth, leading to a high gas content on sidewalls after filling. Option 4 uses a beak-type gate, pouring onto sidewalls of inner shell. While filling is smooth, severe entrapment and entrapment occur, causing rapid temperature drop at entrapment site and posing a significant risk of poor forming and exposed porosity. Therefore, based on mold flow results, Option 2 (flat-bottom center gate) was ultimately chosen for motor inner shell gating system, with gate located on the wall of machined hole at the bottom of inner shell cylinder.
Figure 1 3D diagrams of four different gating schemes
Figure 2 Gas content analysis diagrams of mold flow for four different gating systems
After confirming optimal feed position design (flat-type center gating), slag removal position was designed. Final slag removal position design is shown in Figures 3 and 4. Material particle tracking analysis of gating system in Scheme 2 showed that while a straight-line gating system in the center allows gas in mold cavity to be quickly discharged to exhaust end of motor inner shell, some gas at casting tail impacts and flows back into casting, forming air entrapment and affecting internal density of casting. Therefore, Scheme 2 was further optimized by designing ingate with an angle of <90° to sprue, using a rotary gating method to fill mold cavity. Material particle tracking analysis of mold flow is shown in Figure 4. Molten aluminum is spirally filled inside cylindrical casting of motor inner shell, squeezing out gas in mold. No obvious aluminum backflow was observed, which improves internal density of motor inner shell casting and enhances casting performance.
After confirming optimal feed position design (flat-type center gating), slag removal position was designed. Final slag removal position design is shown in Figures 3 and 4. Material particle tracking analysis of gating system in Scheme 2 showed that while a straight-line gating system in the center allows gas in mold cavity to be quickly discharged to exhaust end of motor inner shell, some gas at casting tail impacts and flows back into casting, forming air entrapment and affecting internal density of casting. Therefore, Scheme 2 was further optimized by designing ingate with an angle of <90° to sprue, using a rotary gating method to fill mold cavity. Material particle tracking analysis of mold flow is shown in Figure 4. Molten aluminum is spirally filled inside cylindrical casting of motor inner shell, squeezing out gas in mold. No obvious aluminum backflow was observed, which improves internal density of motor inner shell casting and enhances casting performance.
Figure 3 Particle tracking diagram of middle linear injection gate (t=0.313 11 s)
Figure 4 Particle tracking diagram of middle rotary injection gate (t=0.375 48 s)
T5 heat treatment of motor inner shell refers to artificial aging treatment after casting has cooled following high-temperature die casting. This process helps to eliminate internal stress generated during casting and improve its mechanical properties. Motor inner shell is made of A380 die-cast aluminum alloy. Mechanical property requirements for sampled casting body are: tensile strength ≥256 MPa, elongation ≥1%, yield strength ≥150 MPa. Natural aging and T5 heat treatment were performed on this motor inner shell, and mechanical properties were measured at same location under six different sample conditions. Results are shown in Table 1. Table 1 shows that mechanical properties of sampled casting body after T5 heat treatment (210 ℃ holding for 75 min + air cooling for 20 min) meet requirements. T5 heat treatment effectively prevents formation of porosity defects by homogenizing internal stress and reducing stress concentration, thereby improving performance of casting.
T5 heat treatment of motor inner shell refers to artificial aging treatment after casting has cooled following high-temperature die casting. This process helps to eliminate internal stress generated during casting and improve its mechanical properties. Motor inner shell is made of A380 die-cast aluminum alloy. Mechanical property requirements for sampled casting body are: tensile strength ≥256 MPa, elongation ≥1%, yield strength ≥150 MPa. Natural aging and T5 heat treatment were performed on this motor inner shell, and mechanical properties were measured at same location under six different sample conditions. Results are shown in Table 1. Table 1 shows that mechanical properties of sampled casting body after T5 heat treatment (210 ℃ holding for 75 min + air cooling for 20 min) meet requirements. T5 heat treatment effectively prevents formation of porosity defects by homogenizing internal stress and reducing stress concentration, thereby improving performance of casting.
| No. | Sample Conditions | Tensile Strength/MPa | Yield Strength/MPa | Elongation/% |
| 1 | Natural Aging 24h | 232.16 | 142.04 | 2.14 |
| 2 | Natural Aging 48h | 252.74 | 138.59 | 3.40 |
| 3 | Natural Aging 72h | 265.12 | 135.56 | 3.56 |
| 4 | Artificial Aging 150℃, 120 min + Air Cooling 20 min | 250.18 | 178.26 | 2.21 |
| 5 | Artificial Aging 180℃, 100 min + Air Cooling 20 min | 255.08 | 177.86 | 1.46 |
| 6 | Artificial Aging 210℃, 75 min + Air Cooling 20 min | 270.17 | 185.68 | 1.89 |
Table 1 Mechanical Properties of Motor Housing Samples
Principle for setting heat fitting temperature is to minimize temperature while ensuring that no scraping occurs during heat fitting process and that assembly is in place, so as to avoid affecting tightness of motor housing. To ensure that inner and outer casings of motor do not interfere with each other during heat fitting, gap between stator holes of inner and outer casings should be controlled within 0.03~-0.07 mm. Conversely, after heat fitting expansion of stator holes of motor housing, hole diameter should be controlled to ϕ209.12~ϕ209.24 mm. Experimental studies on relationship between heat-shrinking temperature and diameter of heat-shrinking hole in motor housing are shown in Figure 5. Inner diameters of holes 1, 2, and 3 are all ϕ248.85 mm, respectively. It was found that when diameter of heat-shrinking hole in motor housing is between ϕ209.12 and ϕ209.24 mm, optimal heating temperature window is 120–140 ℃. Relationship between heating time and temperature is shown in Figure 6. When heat-shrinking temperature is between 120 and 140 ℃, optimal heating time window is 15–19 s.
Principle for setting heat fitting temperature is to minimize temperature while ensuring that no scraping occurs during heat fitting process and that assembly is in place, so as to avoid affecting tightness of motor housing. To ensure that inner and outer casings of motor do not interfere with each other during heat fitting, gap between stator holes of inner and outer casings should be controlled within 0.03~-0.07 mm. Conversely, after heat fitting expansion of stator holes of motor housing, hole diameter should be controlled to ϕ209.12~ϕ209.24 mm. Experimental studies on relationship between heat-shrinking temperature and diameter of heat-shrinking hole in motor housing are shown in Figure 5. Inner diameters of holes 1, 2, and 3 are all ϕ248.85 mm, respectively. It was found that when diameter of heat-shrinking hole in motor housing is between ϕ209.12 and ϕ209.24 mm, optimal heating temperature window is 120–140 ℃. Relationship between heating time and temperature is shown in Figure 6. When heat-shrinking temperature is between 120 and 140 ℃, optimal heating time window is 15–19 s.
Figure 5 Relationship between heating temperature and diameter of heat-shrinking hole in motor housing
Figure 6 Relationship between heating temperature and heating time
During friction stir welding, welding pressure is crucial for obtaining sufficient frictional heat. Simultaneously, pressure limits leakage of plastic fluid and ensures weld formation. Rotational speed and feed rate are main parameters affecting heat input, thus influencing joint performance. For a given shape of friction stir welded joint and assuming good internal quality of casting in welding area, key factors affecting density of weld's internal quality are welding rotational speed, feed rate, and pressure. With other factors remaining constant, orthogonal experiments were conducted on key process parameters (rotational speed, feed rate, and pressure) for friction stir welding of motor housings to determine optimal process parameters. Levels of three factors are shown in Table 2.
Verification was performed using DOE experiments, and results are shown in Table 3. It can be seen that internal quality of motor housing is acceptable under both rotational speed of 750 r/min, feed rate of 250 mm/min, pressure of 0.3 mm, and rotational speed of 850 r/min, feed rate of 350 mm/min, pressure of 0.2 mm. However, latter resulted in severe wear of friction stir welding head. To ensure density of motor housing casting, final selected parameters for friction stir welding were a rotational speed of 750 r/min, a feed rate of 250 mm/min, and a pressure of 0.3 mm.
During friction stir welding, welding pressure is crucial for obtaining sufficient frictional heat. Simultaneously, pressure limits leakage of plastic fluid and ensures weld formation. Rotational speed and feed rate are main parameters affecting heat input, thus influencing joint performance. For a given shape of friction stir welded joint and assuming good internal quality of casting in welding area, key factors affecting density of weld's internal quality are welding rotational speed, feed rate, and pressure. With other factors remaining constant, orthogonal experiments were conducted on key process parameters (rotational speed, feed rate, and pressure) for friction stir welding of motor housings to determine optimal process parameters. Levels of three factors are shown in Table 2.
Verification was performed using DOE experiments, and results are shown in Table 3. It can be seen that internal quality of motor housing is acceptable under both rotational speed of 750 r/min, feed rate of 250 mm/min, pressure of 0.3 mm, and rotational speed of 850 r/min, feed rate of 350 mm/min, pressure of 0.2 mm. However, latter resulted in severe wear of friction stir welding head. To ensure density of motor housing casting, final selected parameters for friction stir welding were a rotational speed of 750 r/min, a feed rate of 250 mm/min, and a pressure of 0.3 mm.
| Horizontal | Rotational speed (A)/(r·min⁻¹) | Feed rate (B)/(mm·min⁻¹) | Indentation (C)/mm |
| 1 | 650 | 150 | 0.1 |
| 2 | 750 | 250 | 0.2 |
| 3 | 850 | 350 | 0.3 |
Table 2 Factor Level Table
| Test No. | Horizontal Combination | Spindle Speed/(r.min) | Feed Rate/(mm.min-1) | Compression/mm | Test Results |
| 1 | A1B1C1 | 650 | 150 | 0.1 | Internal Tunnel, Insufficient Heat Input and Compression |
| 2 | A1B2C2 | 650 | 250 | 0.2 | Internal Tunnel, Insufficient Heat Input |
| 3 | A1B3C3 | 650 | 350 | 0.3 | Internal Tunnel, Insufficient Heat Input |
| 4 | A2B1C2 | 750 | 150 | 0.2 | Internal Tunnel, Insufficient Heat Input |
| 5 | A2B2C3 | 750 | 250 | 0.3 | Internal Quality Qualified |
| 6 | A2B3C1 | 750 | 350 | 0.1 | Internal Tunnel, Insufficient Compression |
| 7 | A3B1C3 | 850 | 150 | 0.3 | Internal Tunnel, Insufficient Heat Input |
| 8 | A3B2C1 | 850 | 250 | 0.1 | Internal Tunnel, Insufficient Compression |
| 9 | A3B3C2 | 850 | 350 | 02 | Internal Quality Qualified |
Table 3 Orthogonal Experiment Results
Conclusion
(1) Inner shell of a new energy vehicle motor adopts a bottom center injection method, with gate designed to have an angle of less than 90° with sprue. Rotary injection is used to fill mold cavity, which solves problem of difficult filling of cylindrical structure of motor inner shell, thereby improving internal density of motor inner shell casting and enhancing its casting performance.
(2) T5 heat treatment (aging temperature 210 ℃, holding for 75 min, air cooling for 20 min) effectively prevents formation of porosity defects by homogenizing internal stress and reducing stress concentration, thus improving performance of motor inner shell.
(3) Hot-fitting pressing process can amplify casting defects, thereby reducing internal density of casting. Hot-fitting pressing process has the least impact on performance of motor inner shell when temperature is 120~140 ℃ and heating time is 15~19 s.
(4) Under premise of a certain shape of stirring head and good internal quality of casting in welding area, key factors affecting internal density of welding area of motor inner shell are welding speed, feed rate and pressure. Through DOE test verification, the internal quality of the welding area of motor inner shell is the best when speed is 750 r/min, feed rate is 250 mm/min and pressure is 0.3 mm, and casting performance is ideal.
Conclusion
(1) Inner shell of a new energy vehicle motor adopts a bottom center injection method, with gate designed to have an angle of less than 90° with sprue. Rotary injection is used to fill mold cavity, which solves problem of difficult filling of cylindrical structure of motor inner shell, thereby improving internal density of motor inner shell casting and enhancing its casting performance.
(2) T5 heat treatment (aging temperature 210 ℃, holding for 75 min, air cooling for 20 min) effectively prevents formation of porosity defects by homogenizing internal stress and reducing stress concentration, thus improving performance of motor inner shell.
(3) Hot-fitting pressing process can amplify casting defects, thereby reducing internal density of casting. Hot-fitting pressing process has the least impact on performance of motor inner shell when temperature is 120~140 ℃ and heating time is 15~19 s.
(4) Under premise of a certain shape of stirring head and good internal quality of casting in welding area, key factors affecting internal density of welding area of motor inner shell are welding speed, feed rate and pressure. Through DOE test verification, the internal quality of the welding area of motor inner shell is the best when speed is 750 r/min, feed rate is 250 mm/min and pressure is 0.3 mm, and casting performance is ideal.
Last article:Introduction to Automatic Descrewing Mechanisms
Next article:Return list
Recommended
Related
- Solving "Internal Damage" Problem of Motor Housings: Rotary Casting + Precision Heat Treat11-23
- Introduction to Automatic Descrewing Mechanisms11-23
- Multi-objective optimization and mold design of two-color injection molding process for air guide ou11-23
- T-slot Driven Slider Design11-21
- Adjustment of Back Pressure in Injection Molding Process11-21