Application of Moldflow in Design of Injection Molds for Rail-Mounted Power Supply Housings
Time:2026-11-25 08:13:38 / Popularity: / Source:
1. Introduction
Process of designing and molding plastic products is highly complex, encompassing several key aspects including product design, mold structure design, mold processing and manufacturing, and mold production. It requires coordinated efforts of product designers, mold designers, mold processing engineers, skilled operators, representing an iterative and continuous optimization process of design, modification, and redesign. Currently, most mold designers rely primarily on their experience to determine mold design schemes. However, due to diversity and complexity of plastic products and limitations of designers' experience, it has long been difficult for engineers to accurately design an optimal process scheme that reduces costs, saves time, improves product quality and yield.
Currently, CAD/CAM is widely used in mold design and manufacturing. However, to design and manufacture high-quality molds, relying solely on CAD/CAM is insufficient; CAE technology is essential. This paper uses Moldflow software to dynamically simulate filling, cooling, and holding pressure processes of a guide rail type power supply housing, providing a theoretical basis for mold design and determination of injection molding process parameters, thereby improving molding quality of plastic parts.
Currently, CAD/CAM is widely used in mold design and manufacturing. However, to design and manufacture high-quality molds, relying solely on CAD/CAM is insufficient; CAE technology is essential. This paper uses Moldflow software to dynamically simulate filling, cooling, and holding pressure processes of a guide rail type power supply housing, providing a theoretical basis for mold design and determination of injection molding process parameters, thereby improving molding quality of plastic parts.
2. Plastic Part Structure and Material Analysis
2.1. Plastic Part Structural Analysis
Figure 1 shows a three-dimensional schematic diagram of rail-mounted power supply casing. Both sides of plastic part have honeycomb-like air inlets and outlets. Due to hook structure at the bottom, wall thickness is locally thicker. Because assembly with power supply cover is directional, openings of casing are partially reduced in thickness to add anti-foolproof notches and stop functions. Its overall dimensions are 75 mm x 72.5 mm x 90 mm, with a maximum wall thickness of 4.0 mm and a minimum wall thickness of 0.5 mm, as shown in Figure 1. This plastic part is an appearance component, requiring a smooth and flat surface, free from obvious weld lines, bubbles, silver streaks, shrinkage cavities, warping, and deformation.
2.2. Plastic Part Material Analysis
Plastic part is made of ABS+PC, with material grade Bayblend FR1514. Material processing parameters are shown in Table 1.
3. Mold Flow Analysis
Plastic part has a symmetrical structure and is an appearance component. Considering that gate could be located either in the middle of outer surface of bottom of product or in the middle of inner surface of bottom of product, a perfect appearance could be achieved, but this would increase mold manufacturing costs. Furthermore, due to limited space in mold core, cooling water channels cannot be arranged. Therefore, gate must be located in the middle of outer surface of bottom of product. Optimal gate location automatically generated by Moldfow is also close to middle of outer surface of bottom of product, as shown in Figure 2, which is basically consistent with initial idea of gate location.
Gate location area on the outer surface of bottom of plastic part is a functional area of product and should not have any gate residue. Considering high appearance requirements of product, hot runner technology is adopted, which can shorten molding cycle, save plastic raw materials, and facilitate production automation. A single-cavity mold layout can meet annual procurement needs of product. Completed gating and cooling systems are shown in Figure 3.
Referring to raw material processing parameter table, process parameters are set as follows: mold surface temperature is 60℃, melt temperature is 260℃, mold opening time is 5s, speed/pressure switching is 97% of filling volume, and holding pressure is 80% of injection pressure. Moldflow analysis sequence is cooling + filling + holding pressure + warpage.
Gate location area on the outer surface of bottom of plastic part is a functional area of product and should not have any gate residue. Considering high appearance requirements of product, hot runner technology is adopted, which can shorten molding cycle, save plastic raw materials, and facilitate production automation. A single-cavity mold layout can meet annual procurement needs of product. Completed gating and cooling systems are shown in Figure 3.
Referring to raw material processing parameter table, process parameters are set as follows: mold surface temperature is 60℃, melt temperature is 260℃, mold opening time is 5s, speed/pressure switching is 97% of filling volume, and holding pressure is 80% of injection pressure. Moldflow analysis sequence is cooling + filling + holding pressure + warpage.
3.1. Filling Analysis
3.1.1. Filling Time Analysis
During plastic melt filling process, filling time is relatively short. As shown in Figure 4, it takes 2.428s for plastic part to be completely filled. However, through animation simulation, it can be seen that plastic melt cannot reach ends of both cavities simultaneously, indicating that product filling is not very balanced.
Table 1. Injection parameter of Bayblend FR1514
During plastic melt filling process, filling time is relatively short. As shown in Figure 4, it takes 2.428s for plastic part to be completely filled. However, through animation simulation, it can be seen that plastic melt cannot reach ends of both cavities simultaneously, indicating that product filling is not very balanced.
Table 1. Injection parameter of Bayblend FR1514
| Mold temperature | Melt temperature | Maximum shear stress | Maximum shear rate | Ejection temperature |
| 70℃ | 260℃ | 0.4 MPa | 20,000/s | 135℃ |
Figure 1. DIN-rail power supply housing 3D
Figure 2. Injection gate matching index
Figure 3. Injection system and cooling system
Figure 4. Fill time
3.1.2. Flow Front Temperature Analysis
Flow front temperature is a crucial indicator of quality of molded part after material filling. After injection molding, a reasonable temperature distribution should be roughly uniform. Allowable temperature difference in mold is generally 20℃. Too low a flow front temperature will result in a poor appearance, an uneven outer wall, and in severe cases, incomplete filling or obvious weld lines. Too high a flow front temperature will lead to material decomposition and may cause residual stress within molded part, which can cause warping and severely affect its quality. As shown in Figure 5, the highest flow front temperature is 274℃, which is within recommended molding temperature range of 250℃ to 280℃ for raw material. However, maximum temperature difference is 34.2℃, indicating an uneven flow front temperature distribution and a lower temperature in grid area.
3.1.3. Weld Line Analysis
When flow fronts of two polymer melts converge, or when a flow front separates and then merges again, weld lines are formed. Weld lines can lead to surface defects and reduced strength in molded part and should be minimized. As shown in Figure 6, weld lines are located in grille area. If unavoidable, this may lead to underfill defects in plastic part.
3.1.4. Cavitation Analysis
Cavitation occurs when there is insufficient plastic in mold cavity. Outer plastic cools and solidifies, causing inner plastic to shrink and create a vacuum. Cavitation may result in incomplete filling of plastic part, leaving air pockets inside; cavitation may also lead to combustion, causing plastic part to char. Cavities should be distributed along boundaries of plastic part, avoiding cavitation on surface A. As shown in Figure 7, cavitation is located in the air vent grille area and is distributed on surface A of plastic part.
3.1.2. Flow Front Temperature Analysis
Flow front temperature is a crucial indicator of quality of molded part after material filling. After injection molding, a reasonable temperature distribution should be roughly uniform. Allowable temperature difference in mold is generally 20℃. Too low a flow front temperature will result in a poor appearance, an uneven outer wall, and in severe cases, incomplete filling or obvious weld lines. Too high a flow front temperature will lead to material decomposition and may cause residual stress within molded part, which can cause warping and severely affect its quality. As shown in Figure 5, the highest flow front temperature is 274℃, which is within recommended molding temperature range of 250℃ to 280℃ for raw material. However, maximum temperature difference is 34.2℃, indicating an uneven flow front temperature distribution and a lower temperature in grid area.
3.1.3. Weld Line Analysis
When flow fronts of two polymer melts converge, or when a flow front separates and then merges again, weld lines are formed. Weld lines can lead to surface defects and reduced strength in molded part and should be minimized. As shown in Figure 6, weld lines are located in grille area. If unavoidable, this may lead to underfill defects in plastic part.
3.1.4. Cavitation Analysis
Cavitation occurs when there is insufficient plastic in mold cavity. Outer plastic cools and solidifies, causing inner plastic to shrink and create a vacuum. Cavitation may result in incomplete filling of plastic part, leaving air pockets inside; cavitation may also lead to combustion, causing plastic part to char. Cavities should be distributed along boundaries of plastic part, avoiding cavitation on surface A. As shown in Figure 7, cavitation is located in the air vent grille area and is distributed on surface A of plastic part.
Figure 5. Temperature at flow front
Figure 6. Welding line
3.2. Cooling Analysis
Quality of cooling system greatly affects molding efficiency and quality of plastic parts. Main influencing factors of cooling system include mold structure, mold size, size of molding projection area, arrangement of gate and runner. Generally, temperature difference between inlet and outlet water should not exceed 5℃. As shown in Figure 8, temperature distribution of coolant in circuit indicates that maximum temperature difference between inlet and outlet is 0.56℃, which is relatively small and meets cooling requirements of plastic parts. As shown in Figure 9, the highest temperature of product after cooling is approximately 86.44℃, which is lower than set ejection temperature of 135℃.
Figure 7. Cavitation
Figure 8. Temperature of cooling lines
3.3. Warpage Analysis
Warpage is a product defect caused by excessive shrinkage. Generally, there are three reasons for excessive shrinkage: uneven cooling, uneven shrinkage in different areas, and molecular inhomogeneity. As shown in Figure 10(c), analysis results show that maximum warpage deformation is 0.5170 mm, of which deformation caused by cooling is very small at 0.0742 mm (Figure 10(a)), and deformation caused by shrinkage is 0.5356 mm (Figure 10(b)). Therefore, shrinkage is main cause of warpage deformation.
Figure 9. Temperature of part after cooling
Figure 10. (a) Deformation caused by uneven cooling: (b) Deformation caused by uneven shrinkage; (c) Deformation caused by all factors
3.3.1. Shrinkage Analysis
As can be seen from mold temperature diagram in Figure 11, mold temperature distribution during injection molding is between 26℃ and 51℃, which does not meet raw material's requirement of 70℃ for mold temperature. A mold temperature controller needs to be used in subsequent actual production. From volume shrinkage rate diagram in Figure 12, it can be seen that shrinkage rate is between -3.660% and 1.746%, exceeding maximum allowable shrinkage rate of raw material. 7%, with larger shrinkage rates concentrated in the end area of part and around gate.
3.3.1. Shrinkage Analysis
As can be seen from mold temperature diagram in Figure 11, mold temperature distribution during injection molding is between 26℃ and 51℃, which does not meet raw material's requirement of 70℃ for mold temperature. A mold temperature controller needs to be used in subsequent actual production. From volume shrinkage rate diagram in Figure 12, it can be seen that shrinkage rate is between -3.660% and 1.746%, exceeding maximum allowable shrinkage rate of raw material. 7%, with larger shrinkage rates concentrated in the end area of part and around gate.
4. Conclusions
Through above simulation analysis, following conclusions can be drawn:
1) Filling analysis shows that although application of hot runner technology improves balance of plastic part filling, due to special structure of product and local asymmetry, uneven filling still occurs. Melt temperature in grid area is low, resulting in poor fluidity and defects such as underfill, weld lines, and air pockets. Furthermore, due to product design requirements, shape, position, and number of grids cannot be changed. Therefore, mold design should focus on adding venting at appropriate locations. During molding, size and position of weld lines can be controlled by adjusting and improving injection molding process, such as increasing injection speed.
2) Cooling analysis shows that cooling of plastic part is relatively uniform, verifying that design and distribution of cooling system are reasonable.
3) Warpage analysis shows that deformation caused by cooling is very small and negligible, further verifying that design of cooling system is sound. Uneven shrinkage is main cause of deformation. Shrinkage rate of a plastic part largely depends on compensating ability of melt, which in turn depends on holding pressure and holding time required to continue transmitting melt into mold at that pressure. This process continues until gate solidifies and closes. Higher holding pressure and longer holding time result in lower shrinkage of plastic part. Therefore, holding pressure and holding time play a crucial role in shrinkage rate of plastic parts.
If shrinkage at the end of plastic part is adjusted, as shown in Figure 13(a), increasing constant pressure duration reduces shrinkage at the end of plastic part, and vice versa.
1) Filling analysis shows that although application of hot runner technology improves balance of plastic part filling, due to special structure of product and local asymmetry, uneven filling still occurs. Melt temperature in grid area is low, resulting in poor fluidity and defects such as underfill, weld lines, and air pockets. Furthermore, due to product design requirements, shape, position, and number of grids cannot be changed. Therefore, mold design should focus on adding venting at appropriate locations. During molding, size and position of weld lines can be controlled by adjusting and improving injection molding process, such as increasing injection speed.
2) Cooling analysis shows that cooling of plastic part is relatively uniform, verifying that design and distribution of cooling system are reasonable.
3) Warpage analysis shows that deformation caused by cooling is very small and negligible, further verifying that design of cooling system is sound. Uneven shrinkage is main cause of deformation. Shrinkage rate of a plastic part largely depends on compensating ability of melt, which in turn depends on holding pressure and holding time required to continue transmitting melt into mold at that pressure. This process continues until gate solidifies and closes. Higher holding pressure and longer holding time result in lower shrinkage of plastic part. Therefore, holding pressure and holding time play a crucial role in shrinkage rate of plastic parts.
If shrinkage at the end of plastic part is adjusted, as shown in Figure 13(a), increasing constant pressure duration reduces shrinkage at the end of plastic part, and vice versa.
Figure 11. Molding temperature
Figure 12. Volume shrinkage rate
Adjusting shrinkage near gate, as shown in Figure 13(b), results in a faster pressure decay and increased shrinkage near gate, and vice versa.
Adjusting shrinkage in the middle region of part, as shown in Figure 13(a), divides pressure decay process into two segments. Adjusting pressure to position shown in figure decreases shrinkage in the middle region, and vice versa.
This part requires reduced shrinkage at ends. During actual molding process, it's important to extend holding time to minimize shrinkage. Simultaneously, a mold temperature controller should be used to heat mold and maintain it at a constant operating temperature to improve balance of filling flow, ensuring sufficient molding shrinkage and reducing subsequent shrinkage.
Adjusting shrinkage near gate, as shown in Figure 13(b), results in a faster pressure decay and increased shrinkage near gate, and vice versa.
Adjusting shrinkage in the middle region of part, as shown in Figure 13(a), divides pressure decay process into two segments. Adjusting pressure to position shown in figure decreases shrinkage in the middle region, and vice versa.
This part requires reduced shrinkage at ends. During actual molding process, it's important to extend holding time to minimize shrinkage. Simultaneously, a mold temperature controller should be used to heat mold and maintain it at a constant operating temperature to improve balance of filling flow, ensuring sufficient molding shrinkage and reducing subsequent shrinkage.
Figure 13. Volume shrinkage rate
5. Conclusion
In summary, based on analysis results of Moldflow's optimal gate location for rail-mounted power supply housing, a preliminary design scheme and corresponding molding simulation results were obtained. Furthermore, simulation results were analyzed to yield corresponding solutions, providing valuable reference and practical guidance for design and modification of molds in actual production.
Recommended
Related
- If mold design facilitation (DFM) isn't done well, T0 trial molding is just a gamble.11-25
- Application of Moldflow in Design of Injection Molds for Rail-Mounted Power Supply Housings11-25
- Automated Molds and Intelligent Molds11-24
- A Step-by-Step Guide to Adjusting Injection Molding Process Parameters – A Must-Read for Machine Tun11-24
- Solving "Internal Damage" Problem of Motor Housings: Rotary Casting + Precision Heat Treat11-23