A Step-by-Step Guide to Adjusting Injection Molding Process Parameters – A Must-Read for Machine Tun
Time:2026-11-24 08:41:05 / Popularity: / Source:
Temperature: Temperature measurement and control are crucial in injection molding. While these measurements are relatively simple, most injection molding machines lack sufficient temperature sampling points or wiring.
On most injection molding machines, temperature is sensed by thermocouples. A thermocouple is essentially composed of two different wires connected at their ends. If one end is hotter than other, a small electrical signal is generated, with signal becoming stronger as heating progresses.
Temperature Control: Thermocouples are also widely used as sensors in temperature control systems. Desired temperature is set on control instrument, and sensor display compares this temperature to temperature at set point. In this simplest system, circuit shuts off when temperature reaches set point and restarts when temperature drops. This system is called on/off control because it is either on or off.
Melt Temperature: Melt temperature is very important; cylinder temperature used is only a guideline. Melt temperature can be measured at nozzle or using an air jet method. Injection cylinder temperature setting depends on melt temperature, screw speed, back pressure, injection volume, and injection cycle.
If you lack experience processing a specific grade of plastic, start with the lowest setting. For ease of control, injection cylinder is divided into zones, but not all zones are set to same temperature. If operating for extended periods or at high temperatures, set first zone temperature to a lower value to prevent premature melting and splitting of plastic. Before injection begins, ensure hydraulic fluid, hopper closure, mold, and injection cylinder are all at correct temperatures.
Injection Pressure: This is pressure that causes plastic to flow and can be measured using sensors on nozzle or hydraulic line. It does not have a fixed value, and the more difficult mold filling, the higher injection pressure. There is a direct relationship between injection line pressure and injection pressure.
First-Stage Pressure and Second-Stage Pressure: During filling phase of injection cycle, high injection pressure may be required to maintain injection speed at required level. High pressure is no longer needed after mold is filled. However, when injection molding some semi-crystalline thermoplastics (such as PA and POM), sudden pressure change can deteriorate structure, so secondary pressure is sometimes unnecessary.
Clamping Pressure: To counteract injection pressure, clamping pressure must be used. Do not automatically select maximum usable value; instead, consider projected area and calculate a suitable value. Projected area of injection molded part is maximum area seen from direction of application of clamping force. For most injection molding cases, it is approximately 2 tons per square inch, or 31 meganewtons per square meter. However, this is a low value and should be used as a very rough rule of thumb because sidewalls must be considered once injection molded part has any depth.
Back Pressure: This is pressure required and exceeded before screw retracts. While high back pressure is beneficial for uniform colorant distribution and plastic melting, it also prolongs screw return time, reduces length of fibers contained in filler plastic, and increases stress on injection molding machine. Therefore, the lower back pressure, the better. Under no circumstances should it exceed 20% of injection pressure (maximum rating) of injection molding machine.
Injection Speed: This refers to filling speed of mold when screw acts as punch. When injection molding thin-walled products, a high injection speed must be used to ensure complete filling of mold before molten plastic solidifies, producing a smoother surface. A series of injection speeds should be used during filling to avoid defects such as jetting or air entrapment. Injection molding can be performed under an open-loop or closed-loop control system.
Regardless of injection speed used, speed value along with injection time must be recorded on a log sheet. Injection time refers to time required for mold to reach predetermined initial injection pressure, which is part of screw advance time.
Mold Venting: Due to rapid filling of mold, mold must allow gas to escape. In most cases, this gas is simply air in mold cavity. If air cannot escape, it will be compressed by melt, causing temperature to rise and potentially leading to plastic combustion. Venting points must be located near watermarks and final injection section. A typical vent is a groove 6 to 13 mm wide and 0.01 to 0.03 mm deep, usually located at parting line of one of mold halves.
Holding Pressure: During filling phase of injection molding cycle, high injection pressure may be required to maintain injection speed at required level. After mold is filled, holding phase begins, where screw (acting as a punch) pushes in additional plastic to compensate for shrinkage. This can be done at a lower or equally high pressure. Generally, if first stage uses high pressure, next stage uses lower pressure. However, when injection molding some semi-crystalline thermoplastics (such as PA and POM), sudden pressure change can deteriorate crystalline structure, so sometimes second stage pressure is unnecessary.
Use of Recycled Plastics: Many injection molding machines use a mixture of virgin material and recycled plastic (commonly known as sprue). Surprisingly, using recycled plastics can improve injection molding machine performance, producing more consistent molded parts. However, it's important to note that recycled material should ideally be dusted before use to avoid variations in plastic feed rate, which can lead to color distribution deviations in molded parts. Exact proportion of recycled plastic used needs to be determined experimentally, and this data must be obtained without affecting physical properties of molded parts; a general rule of thumb is between 15% and 25%.
Quality Control: Final characteristics (weight and size) of injection molded parts are closely related to production conditions such as packing size, injection pressure, and flow rate. This means that in many cases, it's possible to check satisfaction of injection molded parts before any actual measurements are taken. During each injection, selected parameters are measured and compared with set or stored values. As long as measured value is within pre-selected range, control system determines that injection molded part is acceptable. If measurement exceeds set limits, injection molded part will be discarded, or, if it exceeds them only slightly, process will be stopped for a second inspection by qualified personnel. Modern injection molding machines are equipped with video recorders and computer systems, so that each molded part is compared to a stored image of requirements during injection. Each molded part is also compared to a standard injection molded part for dimensions and visual defects.
Recording Injection Conditions: Never forget that purpose of injection molding is to produce molded parts that meet quality requirements within a specified time and at a specified cost. To achieve this, accurate record-keeping is fundamental. This can be done with a button on many injection molding machines. If there is no button, an appropriate record sheet should be completed and injection samples retained for future reference.
Shutting Down: Most importantly, a reasonable shutdown procedure is essential, as this can save significant time and money. If you are shutting down, for example, by burning plastic, then there is no need to vent plastic. You may save cost of completely shutting down and cleaning injection molding machine.
Temporary Stoppages: If injection molding machine is stopped, it is necessary to repeatedly spray out remaining plastic or allow other plastic to pass through injection molding machine to clean remaining plastic in injection cylinder. If plastic is discolored, number of cleaning cycles needs to be increased. When performing minor repairs, injection cylinder heater should be adjusted to the lowest setting to minimize possibility of thermal decomposition. On more modern injection molding machines, this process may start automatically.
Overnight Downtime: Before injection molding thermoplastics (such as PS), if machine has been shut down overnight, simply turn off bottom slide and injection cylinder heater, and thoroughly clean injection cylinder. Clean nozzle completely, cool injection cylinder as much as possible, and once injection molding machine has cooled down, turn off all equipment. Injection molding machine is then ready to be heated again.
Thermoplastics: If plastic decomposes and becomes combustible inside injection molding machine, eventually discoloring and rendering molded part unusable, injection molding machine must be completely shut down and thoroughly cleaned. A preventative measure is to use a heat-stable plastic to clean heat-sensitive plastic, thus allowing for easy reheating after prolonged downtime. To address issue of plastic oxidation, operator can fill injection cylinder with plastic, such as PE.
Important Reasons for Deformation During Plastic Molding
Inconsistent wall thickness and large differences in wall thickness lead to varying shrinkage rates; Uneven injection pressure distribution due to differences in density (gate location and type); Uneven mold temperature distribution, cooling system should be cooler near gate, and vice versa; Excessive differences in molecular orientation; Post-crystallization (in crystalline plastics); Excessive internal stress.
Clamping Pressure: Clamping pressure must be greater than the total pressure of plastic injected into mold. If it is too low, plastic may overflow from parting line. Excessive pressure will damage machine, mold, and waste electricity. Therefore, appropriate clamping force is based on principle that no burrs will appear on parting line after finished product is injected into mold.
Screw Functions: Screw performs functions such as conveying, mixing, venting, dehumidifying, melting, and metering raw materials. Seventy percent of heat required for melting plastic raw materials comes from frictional heat generated during screw rotation, and thirty percent comes from heat supplied by heating elements. For low viscosity, small screws, and high melting speeds, melting speed should be increased. For high viscosity, large screws, and low melting speeds, melting speed should be decreased. Composite materials require slower speeds.
Injection Speed: Injection speed primarily determines flow of raw material in mold's runner and cavity. Too high a speed can cause excessive burrs, burning, and sticking to mold; too low a speed can lead to short shots, shrinkage, and obvious weld lines. Adjustments must be made in stages according to actual needs.
Injection Pressure: Injection pressure and injection speed share some influences, both determining how evenly and thoroughly raw material flows into all corners of mold. Too low a pressure will result in short shots and shrinkage, while too high a pressure will cause burrs, sticking, residual internal stress leading to future deformation, cracking, damage to mold and machine.
Raw Material Temperature: Heat and temperature required for proper melting of raw material during molding. This varies depending on melting temperature and specific heat of each raw material. Too low a temperature results in uneven melting, leading to short shots, uneven color, and high internal stress in finished product. Too high a temperature or too long a heating time can cause burrs on finished product due to its high fluidity, and shrinkage due to temperature differences during cooling. In severe cases, it can cause raw material to decompose, deteriorate, or even burn.
Temperature Control: Thermocouples are also widely used as sensors in temperature control systems. Desired temperature is set on control instrument, and sensor display compares this temperature to temperature at set point. In this simplest system, circuit shuts off when temperature reaches set point and restarts when temperature drops. This system is called on/off control because it is either on or off.
Melt Temperature: Melt temperature is very important; cylinder temperature used is only a guideline. Melt temperature can be measured at nozzle or using an air jet method. Injection cylinder temperature setting depends on melt temperature, screw speed, back pressure, injection volume, and injection cycle.
If you lack experience processing a specific grade of plastic, start with the lowest setting. For ease of control, injection cylinder is divided into zones, but not all zones are set to same temperature. If operating for extended periods or at high temperatures, set first zone temperature to a lower value to prevent premature melting and splitting of plastic. Before injection begins, ensure hydraulic fluid, hopper closure, mold, and injection cylinder are all at correct temperatures.
Injection Pressure: This is pressure that causes plastic to flow and can be measured using sensors on nozzle or hydraulic line. It does not have a fixed value, and the more difficult mold filling, the higher injection pressure. There is a direct relationship between injection line pressure and injection pressure.
First-Stage Pressure and Second-Stage Pressure: During filling phase of injection cycle, high injection pressure may be required to maintain injection speed at required level. High pressure is no longer needed after mold is filled. However, when injection molding some semi-crystalline thermoplastics (such as PA and POM), sudden pressure change can deteriorate structure, so secondary pressure is sometimes unnecessary.
Clamping Pressure: To counteract injection pressure, clamping pressure must be used. Do not automatically select maximum usable value; instead, consider projected area and calculate a suitable value. Projected area of injection molded part is maximum area seen from direction of application of clamping force. For most injection molding cases, it is approximately 2 tons per square inch, or 31 meganewtons per square meter. However, this is a low value and should be used as a very rough rule of thumb because sidewalls must be considered once injection molded part has any depth.
Back Pressure: This is pressure required and exceeded before screw retracts. While high back pressure is beneficial for uniform colorant distribution and plastic melting, it also prolongs screw return time, reduces length of fibers contained in filler plastic, and increases stress on injection molding machine. Therefore, the lower back pressure, the better. Under no circumstances should it exceed 20% of injection pressure (maximum rating) of injection molding machine.
Injection Speed: This refers to filling speed of mold when screw acts as punch. When injection molding thin-walled products, a high injection speed must be used to ensure complete filling of mold before molten plastic solidifies, producing a smoother surface. A series of injection speeds should be used during filling to avoid defects such as jetting or air entrapment. Injection molding can be performed under an open-loop or closed-loop control system.
Regardless of injection speed used, speed value along with injection time must be recorded on a log sheet. Injection time refers to time required for mold to reach predetermined initial injection pressure, which is part of screw advance time.
Mold Venting: Due to rapid filling of mold, mold must allow gas to escape. In most cases, this gas is simply air in mold cavity. If air cannot escape, it will be compressed by melt, causing temperature to rise and potentially leading to plastic combustion. Venting points must be located near watermarks and final injection section. A typical vent is a groove 6 to 13 mm wide and 0.01 to 0.03 mm deep, usually located at parting line of one of mold halves.
Holding Pressure: During filling phase of injection molding cycle, high injection pressure may be required to maintain injection speed at required level. After mold is filled, holding phase begins, where screw (acting as a punch) pushes in additional plastic to compensate for shrinkage. This can be done at a lower or equally high pressure. Generally, if first stage uses high pressure, next stage uses lower pressure. However, when injection molding some semi-crystalline thermoplastics (such as PA and POM), sudden pressure change can deteriorate crystalline structure, so sometimes second stage pressure is unnecessary.
Use of Recycled Plastics: Many injection molding machines use a mixture of virgin material and recycled plastic (commonly known as sprue). Surprisingly, using recycled plastics can improve injection molding machine performance, producing more consistent molded parts. However, it's important to note that recycled material should ideally be dusted before use to avoid variations in plastic feed rate, which can lead to color distribution deviations in molded parts. Exact proportion of recycled plastic used needs to be determined experimentally, and this data must be obtained without affecting physical properties of molded parts; a general rule of thumb is between 15% and 25%.
Quality Control: Final characteristics (weight and size) of injection molded parts are closely related to production conditions such as packing size, injection pressure, and flow rate. This means that in many cases, it's possible to check satisfaction of injection molded parts before any actual measurements are taken. During each injection, selected parameters are measured and compared with set or stored values. As long as measured value is within pre-selected range, control system determines that injection molded part is acceptable. If measurement exceeds set limits, injection molded part will be discarded, or, if it exceeds them only slightly, process will be stopped for a second inspection by qualified personnel. Modern injection molding machines are equipped with video recorders and computer systems, so that each molded part is compared to a stored image of requirements during injection. Each molded part is also compared to a standard injection molded part for dimensions and visual defects.
Recording Injection Conditions: Never forget that purpose of injection molding is to produce molded parts that meet quality requirements within a specified time and at a specified cost. To achieve this, accurate record-keeping is fundamental. This can be done with a button on many injection molding machines. If there is no button, an appropriate record sheet should be completed and injection samples retained for future reference.
Shutting Down: Most importantly, a reasonable shutdown procedure is essential, as this can save significant time and money. If you are shutting down, for example, by burning plastic, then there is no need to vent plastic. You may save cost of completely shutting down and cleaning injection molding machine.
Temporary Stoppages: If injection molding machine is stopped, it is necessary to repeatedly spray out remaining plastic or allow other plastic to pass through injection molding machine to clean remaining plastic in injection cylinder. If plastic is discolored, number of cleaning cycles needs to be increased. When performing minor repairs, injection cylinder heater should be adjusted to the lowest setting to minimize possibility of thermal decomposition. On more modern injection molding machines, this process may start automatically.
Overnight Downtime: Before injection molding thermoplastics (such as PS), if machine has been shut down overnight, simply turn off bottom slide and injection cylinder heater, and thoroughly clean injection cylinder. Clean nozzle completely, cool injection cylinder as much as possible, and once injection molding machine has cooled down, turn off all equipment. Injection molding machine is then ready to be heated again.
Thermoplastics: If plastic decomposes and becomes combustible inside injection molding machine, eventually discoloring and rendering molded part unusable, injection molding machine must be completely shut down and thoroughly cleaned. A preventative measure is to use a heat-stable plastic to clean heat-sensitive plastic, thus allowing for easy reheating after prolonged downtime. To address issue of plastic oxidation, operator can fill injection cylinder with plastic, such as PE.
Important Reasons for Deformation During Plastic Molding
Inconsistent wall thickness and large differences in wall thickness lead to varying shrinkage rates; Uneven injection pressure distribution due to differences in density (gate location and type); Uneven mold temperature distribution, cooling system should be cooler near gate, and vice versa; Excessive differences in molecular orientation; Post-crystallization (in crystalline plastics); Excessive internal stress.
Clamping Pressure: Clamping pressure must be greater than the total pressure of plastic injected into mold. If it is too low, plastic may overflow from parting line. Excessive pressure will damage machine, mold, and waste electricity. Therefore, appropriate clamping force is based on principle that no burrs will appear on parting line after finished product is injected into mold.
Screw Functions: Screw performs functions such as conveying, mixing, venting, dehumidifying, melting, and metering raw materials. Seventy percent of heat required for melting plastic raw materials comes from frictional heat generated during screw rotation, and thirty percent comes from heat supplied by heating elements. For low viscosity, small screws, and high melting speeds, melting speed should be increased. For high viscosity, large screws, and low melting speeds, melting speed should be decreased. Composite materials require slower speeds.
Injection Speed: Injection speed primarily determines flow of raw material in mold's runner and cavity. Too high a speed can cause excessive burrs, burning, and sticking to mold; too low a speed can lead to short shots, shrinkage, and obvious weld lines. Adjustments must be made in stages according to actual needs.
Injection Pressure: Injection pressure and injection speed share some influences, both determining how evenly and thoroughly raw material flows into all corners of mold. Too low a pressure will result in short shots and shrinkage, while too high a pressure will cause burrs, sticking, residual internal stress leading to future deformation, cracking, damage to mold and machine.
Raw Material Temperature: Heat and temperature required for proper melting of raw material during molding. This varies depending on melting temperature and specific heat of each raw material. Too low a temperature results in uneven melting, leading to short shots, uneven color, and high internal stress in finished product. Too high a temperature or too long a heating time can cause burrs on finished product due to its high fluidity, and shrinkage due to temperature differences during cooling. In severe cases, it can cause raw material to decompose, deteriorate, or even burn.
Mold Temperature: Raw material injects a large amount of heat into mold, while finished product dissipates some of that heat into air. Therefore, to maintain a constant mold temperature, chilled water, cold water, hot water, hot oil, or heating rods are circulated within mold to achieve thermal balance between material entering and exiting mold, thus maintaining a constant temperature. If mold temperature is too low, finished product is prone to short shots, rough surfaces, high internal stress, and sticking to mold. If mold temperature is too high, finished product is prone to shrinkage and sinking, and production cycle is prolonged. Therefore, cooling time and mold temperature can be set based on experience.
Recommended
Related
- Automated Molds and Intelligent Molds11-24
- A Step-by-Step Guide to Adjusting Injection Molding Process Parameters – A Must-Read for Machine Tun11-24
- Solving "Internal Damage" Problem of Motor Housings: Rotary Casting + Precision Heat Treat11-23
- Introduction to Automatic Descrewing Mechanisms11-23
- Multi-objective optimization and mold design of two-color injection molding process for air guide ou11-23